Cross-reference tables for DIN aluminium wrought alloys: Part 1


Resumé:
Cross-reference tables between alphanumeric and numeric temper designations for wrought aluminum alloys according to DIN 1788 and DIN 1790 standard specifications are given in this article. It covers sheets and strips with thickness from 0,021 to 0,035mm and aluminium alloy wires.

DIN 1788

Sheet and strip of wrought aluminum and aluminum alloys, with thickness from 0.021 to 0.350 mm, mechanical properties

Alphanumeric designation (Kurzzeichen) Numeric designation
(Werkstoff-nummer)
AI99,98R W4 3.0385.10
F14 .32
Al99,5 W6 3.0255.10
W7 .10
F9 .24
F11 .26
G11 .27
F13 .30
G13 .31
F15 .32
F18 .34
Al99 W6 3.0205.10
W7 .10
W8 .10
F12 .26
F14 .30
F16 .32
F19 .34
AlFeSi W8 3.0915.10
F11 .24
G11 .25
F13 .26
G13 .27
F15 .28
G15 .29
F17 .30
F20 .32
AlMnCu W10 3.0517.10
G13 .25
F15 .26
G15 .27
F17 .28
G17 .29
F19 .30
AlMn0.5Mg0.5 W11 3.0505.10
G16 .25
F17 .26
G17 .27
F20 .28
G20 .29
F22 .30
F24 .32
AlMn1Mg0,5 W13 3.0525.10
G17 .25
G21 .31
F25 .32
AlMn1Mg1 W16 3.0526.10
F19 .24
G19 .25
F21 .26
G21 .27
F23 .28
G23 .29
F25 .30
G25 .31
F28 .32
AlMg1 W11 3.3315.10
G12 .25
F15 .26
G15 .27
F17 .28
F19 .30
F22 .32
AlMg2,5 W18 3.3523.10
G26 .29
F32 .34
AlMg3 W19 3.3535.10
F24 .26
G24 .27
F27 .28
G27 .29
F29 .30
G29 .31
F32 .32
AlMg4,5 G34 3.3345.31
F37 .32
G37 .33

DIN 1790

Wire of wrought aluminum and aluminum alloys; mechanical properties

Alphanumeric designation (Kurzzeichen) Numeric designation
(Werkstoff-nummer)
Al99,8R W4 3.0385.10
F7 .26
F11 .30
Al99,9 W4 3.0305.10
F7 .26
F11 .30
Al99,8 W6 3.0285.10
F9 .26
F12 .30
Al99,5 W7 3.0255.10
F10 .26
F14 .30
Al99 W8 3.0205.10
F11 .26
F15 .30
Al99,9Mg0,5 W7 3.3308.10
F10 .26
F13 .30
Al99,9Mg1 W10 3.3318.10
F13 .26
F16 .30
Al99,85Mg0,5 W7 3.3307.10
F10 .26
F13 .30
Al99,85Mg1 W10 3.3317.10
F13 .26
F16 .30
AlMn W10 3.0515.10
F13 .26
F16 .30
AlMg1 W10 3.3315.10
F14 .26
F19 .30
AlMg2Mn0,3 W15 3.3525.10
F19 .24
F23 .28
G22 .29
AlMg2,5 W17 3.3523.10
F21 .24
F25 .28
G24 .29
AlMg3 W18 3.3535.10
F23 .24
F27 .28
G26 .29
AlMg5 W27 3.3555.10
F31 .26
F35 .30
G34 .31
AlMgsSi0,5 W9 3.3206.10
F12 .26
F15 .41
F20 .53
F22 .61
F27 .56
F30 .73
AlMgSi1 W11 3.2315.10
F15 .26
F20 .41
F25 .53
F28 .61
F32 73
AlCu2,5Mg0,5 F18 3.1305.26
F27 .41
F31 .53
AlCuMg1 F22 3.1325.26
F38 .41
F42 .53
AlCuMg2 F26 3.1355.26
F42 .41
F48 .53
AlZn4,5Mg1 F35 3.4335.61
AlZnMgCu0,5 F20 3.4345.26
F46 .46
AlZnMgCu1,5 F25 3.4365.26
F51 .61
F55 .73


Date Published: Jun-2002