Complex Phase Steels


Sommario:
Complex-phase steels display high fatigue strength. Based on stress-strain curves they display higher fatigue strength than dual-phase and retained austenite steels, but they are more sensitive to severe strain peaks, i.e. abusive loads.
The structure of the steels is a ferrite/bainite matrix containing martensite and small amounts of retained austenite and/or perlite. This creates a high yield strength tensile strength ratio.

The complex-phase (CP) steels belong to the group of AHSS grade, which gain their strength through extremely fine grain size and a microstructure containing bainite, martensitic, retained austenite and pearlite. These steel grades have been used for parts that require high energy-absorption capacity, such as bumpers and B-pillar reinforcements.

Complex – phase steels can be welded to other complex-phase steels and to other common steel grades. The welding parameters must be matched to the material. To spot-weld complex-phase steels the same equipment can generally be used as for unalloyed deep-drawing steels.

Compared with lower-strength steel grades, complex-phase steels tend to have a lower electrical conductivity, which is why they require lower welding current with the same electrode force in spot welding. When resistance spot welding galvanises sheets, the welding currents must be raised due to the higher conductivity of the coating compared with the base metal. In addition, increasing the electrode force and welding time has a favorable effect on the welding current range.

As well as sheet grade, surface and thickness ratio, other factors such as the type of electrode used play an important role in determining the optimum joining parameters.

Fatigue strength

Complex-phase steels display high fatigue strength. Based on stress-strain curves they display higher fatigue strength than dual-phase and retained austenite steels, but they are more sensitive to severe strain peaks, i.e. abusive loads.

As an illustration of CP steel grades, please note some information about these materials produced by well known producers.

Dogal CP (Complex Phase steels) are cold-rolled advanced high strength steels, which are hot-dip galvanized for corrosion protection. Dogal CP grades are multiphase steels. The structure of the steels is a ferrite/bainite matrix containing martensite and small amounts of retained austenite and/or perlite.

This creates a high yield strength tensile strength ratio. Generally CP steels are easy to cold-form and excellent for stretch forming and roll forming. The steel grades are supplied in accordance with EN 10336.

Also, ThyssenKrupp supplies two hot-rolled grades and one cold-rolled grade with strengths between 800 MPa and 1,000 MPa. Strip can be supplied in thicknesses between 0.8 and 3.0 mm and with two different coatings.

Tables 1, 2 and 3 give some common information about ThyssenKrupp steel grades.

ThyssenKrupp Steel   EN 10336
Hot rolled CP-W®800 HDT 780C
Hot rolled CP-W®1000 HDT 950C
Cold rolled CP-K®60/78 HCT 780C
Cold rolled CP-K®70/98 HCT 980C

Table 1: Steel grade designations

Steel grade   %C
max
%Si
max
%Mn
max
%P
max
%S
max
%Cr+%Mo
max
%Nb+%Ti
max
%Al
max
%V
max
%B
max
CP-W®800 Hot rolled 0.12 0.80 2.20 0.04 0.015 1.00 0.15 1.20 0.20 0.005
CP-W®1000 Hot rolled 0.17 0.80 2.20 0.04 0.015 1.00 0.15 1.20 0.20 0.005
CP-K®60/78 Cold rolled 0.12 0.80 2.20 0.04 0.015 1.00 0.15 1.20 0.20 0.005

Table 2: Chemical composition (ladle analysis in wt.%)

Steel grade σ0.2
MPa
σm
MPa
Elongation
A80, % min
CP-W®800 680-830 800-980 10
CP-W®1000 720-920 950-1130 10
CP-K®60/78 600-700 780-940 10

Table 3: Mechanical properties for uncoated sheet (transverse)

Complex Phase steels exhibit good fatigue properties and can be used in suspension system parts such as suspension arms. The figure below gives examples of Wöhler curves for a variety of Complex Phase steels produced by ArcellorMittal. They are expressed as stress amplitude versus cycles to failure and are obtained with a stress ratio of R = 0.1 and repeated tensile loading.



Figure 1: Wöhler or SN curves for Complex Phase steels (R=0.1)

The graph below shows the low cycle or EN curves for the same steels. These are expressed as strain amplitude versus number of reversals (one cycle equals two reversals). Other high and low cycle fatigue data are available on request.



Figure 2: Low cycle or EN curves for Complex Phase steels (R=-1)


Date Published: Jun-2012




Il database KEY to METALS database riporta proprietà del metallo a livello mondiale insieme in un unico database integrato e la ricerca. Rapido e facile accesso alle proprietà meccaniche, composizione chimica, le tabelle di riferimenti incrociati e più fornire agli utenti una ricchezza di informazioni senza precedenti. Fare clic sui pulsanti qui sotto per saperne di più dalla visita guidata o per provare la KEY to METALS database.